Compound Test Specifications
RECIPE: V6034-SPDA BASE POLYMER: EPDM/CPE
SPECIFICATION BASIS: ASTM D-1056, Grade 2A2 & 2C2
|
METHOD
|
SPECIFICATION
|
REQUIRED
|
OBTAINED
|
|
D-1056-B
|
Compression Set, %
max, 22h @ RT, 50%
deflection, 24h recov.
|
25%
|
8.1
|
|
D-1056
|
Compression Deflection
@ 25% deflection.
|
5-9 psi
|
8.4
|
|
|
Heat aged 168h @ 158º
max load increase to
deflect 25%. D-573
|
25%
|
2.6
|
|
|
Shrinkage, 50h @ 93ºC
|
5% max
|
-3.4
|
|
D-1056
|
Water Absorbtion,
Mass % change.
|
+5%
|
1.04
|
|
D-1149
|
Ozone resistance 72h @
38ºC, 20% stretch,
100 pphm
|
no cracks
|
no cracks
|
|
|
Flammability, not able
to support combustion
after ignition.
|
no burn
|
pass
|
|
D-1056
|
Oil resistance 7 days at
23ºC (73.4ºF) change in
weight, Fuel B.
|
150% max
|
94%
|